Rust dip success stories?

Things I have found that help the electrolysis process. Use hot water for the medium mixed with washing soda. Non pulsing dc power supplies (laboratory grade) work better than a battery charger. When using a battery charger, You can stop the pulsing by hooking up a car battery between the anode and electrode. Use graphite for your sacrificial anode, the bigger the better. I have 4 around the perimeter of the bucket 2x4x1/4 in size. Graphite will degrade slower than steel and will not have scum buildup on top of the water medium. Never use or derust chrome plated objects, it produces toxic and carcinogenic gases. Hexavalent chromium.